micrometer gauge, whilst the wall thickness measurements  for 2 mm cylinder was done using Ultrasonic thickness measurement gauge。 The wall thickness was measured at eleven different equi- distance points along the axial length of the cylinder。 This was then repeated along 36° spaced along the circumference of the cylinder, resulting in 11 ~ 10 ¼ 110 measuring points。 The nominal tnom, average tave, minimum tmin and maximum tmax wall thickness and the corresponding standard deviation for all specimens   are

shown in Table 2。 Next, both the inner and outer diameters of the cylinders were measured at five equally spaced diameters using digital vernier caliper at the top and bottom ends respectively。 The average mid-surface diameter at the top and bottom and the corresponding standard deviation for all cylinders are shown in Table 3。 Lastly, the axial lengths of all cylinders were measured using digital Vernier caliper at eleven equidistance point。 The corresponding average lengths and standard deviation are also shown in Table  3。

Finally, all cylindrical specimens (CY1_t0。5, CY1_t1。0, CY2_t1。0, CY1_t2。0 and CY2_t2。0) were subjected to axial compression using Universal Instron Machine。 Specimen was placed between the platens of INSTRON machine without any clamping plates, as shown in Fig。 3a for 2 mm cylindrical specimen。 Then, the movable crosshead is gently adjusted until a contact is established between the specimen and the instron platen, as depicted in Fig。 3b。 It is assumed that the platen of the INSTRON machine will helps to provide the desirable boundary condition。 Though it is practically impossible to achieve fully clamped condition without rotation, but the effect of rotation on the magnitude of buckling load of cylindrical shell has been proven to be marginal [17]。 The same experimental set up was repeated for 0。5 mm and 1 mm cylinder。 Incremental axial load was applied to one side of the cylindrical specimen at the rate of 1。0 mm/min。 This is the same rate of loading used to obtain the material properties of the mild steel plate from which the cylinders were made。 The compression ex- tension and the corresponding load at each increment were measured by the machine。 Fig。 4 shows a typical curve of load versus compression extension for cylinder with different radius- to-thickness ratio, R/t。 It can be seen from Fig。 4, that the load deflection curve is nearly linear up to the failure load。 Again, it is apparent from Fig。 4, that increasing the thickness of the cylinder

results in an increase in the stiffness of the   material。

Table 3

Measured average data and standard deviation of mid-surface top and bottom diameter and axial length for all tested cylinders。 Note: D ≡average mid-surface diameter, ΔD≡

standard deviation for mid-surface diameter。

Dtop Δ¯Dtop

Dbottom Δ¯Dbottom Lave Lstd Dtop /tave Lave/ Dtop

(mm)

CY1_t0。5 102。02 0。963 101。55 0。732 113。06 0。0954 204。04 1。108

CY1_t1。0 101。54 0。146 101。04 0。067 112。4

上一篇:基卡气体管道PLEM结构的原状分析英文文献和中文翻译
下一篇:加压蛋壳分析英文文献和中文翻译

压缩机壳体用铝合金英文文献和中文翻译

加压蛋壳分析英文文献和中文翻译

单级直齿圆柱齿轮减速器英文文献和中文翻译

Moldflow软件在复杂的塑料外...

减速起动机行星轮销轴压...

圆柱尾迹的时空结构英文文献和中文翻译

齿轮箱外壳综合设置和夹...

酵母菌发酵生产天然香料...

基于Joomla平台的计算机学院网站设计与开发

上海居民的社会参与研究

压疮高危人群的标准化中...

从政策角度谈黑龙江對俄...

浅谈高校行政管理人员的...

AES算法GPU协处理下分组加...

提高教育质量,构建大學生...

STC89C52单片机NRF24L01的无线病房呼叫系统设计

浅论职工思想政治工作茬...